The L in 316L is a carbon limit: 0.03% maximum in plate to ASTM A240, against 0.08% for plain 316. Sanitary tube to ASTM A270 allows 0.035%.
Welding heats the metal beside the bead, the heat-affected zone, through roughly 425 to 815 °C. In that range, carbon combines with chromium and precipitates as chromium carbide along the grain boundaries. Chromium tied up in carbide no longer supports the passive film, so a thin band either side of the weld loses corrosion resistance. Metallurgists call it sensitization.
Holding carbon that low leaves too little of it to form much carbide in the short time a weld spends in the range, so the joint keeps its chromium. That is why PW and WFI piping is specified in 316L.
Low carbon handles one failure mechanism. In thin-wall orbital-welded tube, heat tint from a poor purge and incomplete passivation are more common starting points for rouge and pitting, so the weld procedure, the purge and the passivation record need the same attention as the grade.
The mill certificate is where the grade is proven, and the carbon figure has to be read against the product form. A tube certificate showing 0.034% is within A270; the same figure on plate would fail A240.
On the equipment we supply, material certificates and weld and passivation records go into the equipment file during production, so IQ starts from a complete record.